Example 6: Cut speed increased from 1800 mm/min (72 in./min) to 2080 mm/min (82 in./min)
In this example, the top lines are not bad. However, the bottom lines are trailing and inconsistent. Also, there is a lack of
oxygen at the bottom of the cut.
thickness
Nozzle
Cut parameters
type and
size (mm)
Nozzle
extension
Creep
time
Cut
pressure
Cut
height
Kerf
width
Cut
power
Cut
speed
6 mm
(0.25 in.)
D1.5
23 mm
0.2 sec
0.55 bar
(8 psi)
1 mm
(0.04 in.)
0.35 mm
(0.014 in.)
2000 W
2080 mm/min
(82 in./min)
Cut direction
Example 7: Cut speed decreased from 1800 mm/min (72 in./min) to 1016 mm/min (40 in./min)
In this example, the cut is very consistent from the top to the bottom. However, decreasing the cut rate reduces
productivity. The operator needs to reach a balance between cut quality and productivity.
thickness
Nozzle
Cut parameters
type and
size (mm)
Nozzle
extension
Creep
time
Cut
pressure
Cut
height
Kerf
width
Cut
power
Cut
speed
6 mm
(0.25 in.)
D1.5
23 mm
0.2 sec
0.55 bar
(8 psi)
1 mm
(0.04 in.)
0.35 mm
(0.014 in.)
2000 W
1016 mm/min
(40 in./min)
Cut direction