Ivoclar Vivadent IPS e.max CAD-on User Manual
Page 41
41
Do not remove IPS Object Fix Putty or Flow residues with Al
2
O
3
or glass polishing beads.
Check the shade with the Shade Guide.
Completed IPS e.max CAD-on restoration on the model.
Glaze,
Characterization
Furnace
P300
P500
P700
EP 5000
B
[°C/°F]
403/757
S
[min]
6:00
t
1
[°C/°F/min]
60/108
T
1
[°C/°F]
820/1508
H
1
[min]
00:10
t
2
[°C/°F/min]
30/54
T
2
[°C/°F]
840/1544
H
2
[min]
03:00
V1
1
/
V1
2
[°C/°F]
550/820
1022/1508
V2
1
/
V2
2
[°C/°F]
820/840
1508/1544
L
[°C/°F]
600/1112
t
l
[°C/°F/min]
0
Firing parameters: IPS e.max CAD-on technique Characterization/Glaze firing
Once the IPS e.max CAD-on restoration has cooled to room temperature, proceed with the following steps:
– Remove the restoration from the IPS e.max CAD Crystallization Tray.
– Remove adhering IPS Object Fix Putty or Flow residue with ultrasound in a water bath and/or with steam.
– Do not blast IPS Object Fix Putty or Flow residue with Al
2
O
3
or glass polishing beads.
– Check the fit on the model and in the articulator. For bridges, pay particular attention to the fit of the bridge pontic on
the "gingiva".
– If adjustments by grinding are required, use suitable grinding instruments. Observe the recommendations regarding the
selection of suitable grinding tools.