IPS e.max Ceram on Zenostar T – Staining Technique

IPS e.max Ceram

B

°C

S

min

t

°C/min

T

°C

H

min

V1

°C

V2

°C

Stain and
Characterization firing

403

6:00

60

770

1:00

450

769

Glaze firing

403

6:00

60

770

1:00-

2:00

450

769

Add-on after Glaze firing

403

6:00

50

770

1:00

450

699

If several objects (multi-unit bridges with massive bridge pontics or several full-contour restorations) are fired in one firing cycle, the
heating of the objects in the furnace may be delayed. This delay can be counteracted by either reducing the heating rate or by
extending the holding time at the final temperature.

The heating of the firing chamber depends on the type of furnace as well as the size of the firing chamber!

Firing parameters for IPS e.max Ceram

IPS e.max Ceram on Zenostar T/MO – Layering Technique

IPS e.max Ceram

B

°C

S

min

t

°C/min

T

°C

H

min

V1

°C

V2

°C

L

°C

ZirLiner firing

403

4:00

40

960

1:00

450

959

0

1

st

Margin firing

403

4:00

40

800

1:00

450

799

0

2

nd

Margin firing

403

4:00

40

800

1:00

450

799

0

Wash firing

403

4:00

40

750

1:00

450

749

0

1

st

Dentin-/Incisal firing

403

4:00

40

750

1:00

450

749

0

2

nd

Dentin-/Incisal firing

403

4:00

40

750

1:00

450

749

0

Stain firing

403

4:00

60

725

1:00

450

724

450

Glaze firing

403

4:00

60

725

1:00

450

724

450

Add-on with Glaze firing

403

4:00

60

725

1:00

450

724

450

Add-on after Glaze firing

403

4:00

50

700

1:00

450

699

450