5 Non-metallic particles

are trapped in the
weld metal (slag
inclusion).

A Non-metallic particles may be

trapped in undercut from
previous run.

A If bad undercut is present, clean

slag out and cover with a run
from a smaller diameter electrode.

B Joint preparation too restricted.

B Allow for adequate penetration

and room for cleaning out
the slag.

C Irregular deposits allow slag to

be trapped.

C If very bad, chip or grind out

irregularities.

D Lack of penetration with slag

trapped beneath weld bead.

D Use smaller electrode with

sufficient current to give adequate
penetration. Use suitable tools to
remove all slag from corners.

E Rust or mill scale is preventing

full fusion.

E Clean joint before welding.

F Wrong electrode for position in

which welding is done.

F Use electrodes designed for

position in which welding is done,
otherwise proper control of slag
is difficult.

Figure 10. Examples of Slag Inclusion