WELD DIAGNOSIS

ExCESS OR BURN-THROUGH

Weld droops on top and

underneath, or falls through

entirely, making a hole.

PROPER

Weld is visible underneath and

bulges slightly on top.

INADEqUATE

Weld does not contact the joint

fully, just on the surface.

WELD PENETRATION

POSSIBLE CAUSES AND SOLUTIONS

1.

Excessive material at weld:

Reduce wire feed speed.

2.

Overheating:

Increase welding speed and ensure that

welding speed is kept steady.

POSSIBLE CAUSES AND SOLUTIONS

1.

Workpieces too thick/close:

Joint design must allow weld to reach bot-

tom of groove and allow proper welding

procedures.

2.

Incorrect welding technique:

Maintain

1

/

2

” or less stickout.

Keep arc on leading edge of weld pud-

dle.

Hold gun at proper angles as stated under

Holding The Torch on page 17.

3.

Insufficient weld material:

Increase wire feed speed.

4.

Insufficient weld heat:

Reduce Welding Speed.

Cross seCtIons

WELD NOT ADHERING PROPERLY

Gaps present between weld and previous bead or

between weld and workpiece. See areas below.

POSSIBLE CAUSES AND SOLUTIONS

1.

Dirty workpiece:

Make certain that workpiece is clean and

free from oil, coatings, and other resi-

dues.

2.

Insufficient weld material:

Increase wire feed speed.

3.

Incorrect welding technique:

Place stringer bead at correct place in

joint.

Adjust workpiece position or weld angle to

permit proper welding to bottom of piece.

Pause briefly at sides when using a weave

bead.

Keep arc on leading edge of weld

puddle.

Hold gun at proper angles as stated under

Holding The Torch on page 17.

Cross

seCtIon

BEND AT jOINT

POSSIBLE CAUSES AND SOLUTIONS

1.

Improper clamping:

Make sure that pieces are clamped se-

curely in place.

Make tack welds to help hold pieces.

2.

Excessive heat:

Weld a small portion and allow to cool

before proceeding.

Reduce wire feed speed.

Increase weld speed.

Cross