Powermax – Hypertherm Powermax65 Service Manual Rev.1 User Manual
Page 89
![background image](https://www.manualsdir.com/files/789800/content/doc089.png)
Torch SeTup
powermax
65/85 Service Manual
3-41
Low Speed FineCut
Air flow rate – slpm/scfh
Mild Steel
Hot
155 / 330
Cold
215 / 460
Metric
Material
Thickness
Current
Torch-
to-Work
Distance
Initial Pierce Height
Pierce Delay
Time
Recommended
Cut Speed
Voltage
mm
A
mm
mm
%
seconds
(mm/min)
Volts
0.5
30
1.5
2.25
150
0.0
3800
69
0.6
3800
68
0.8
0.1
3800
70
1 *
40
0.2
3800
72
1.5 *
0.4
3800
75
2
45
3700
76
3
0.5
2750
78
4
1900
78
English
Material
Thickness
Current
Torch-
to-Work
Distance
Initial Pierce Height
Pierce Delay
Time
Recommended
Cut Speed
Voltage
A
inches
inches
%
seconds
ipm
Volts
26GA
30
0.06
0.09
150
0.0
150
70
24GA
150
68
22GA
0.1
150
70
20GA
150
71
18GA
40
0.2
150
73
16GA *
0.4
150
75
14GA *
45
150
76
12GA
0.5
120
78
10GA
95
78
*Not a dross-free cut.